Supporting > Casting
Cast iron porosity.
CI:
This is one of the castings made from the molds in the video above.
The surface irregularity is quite odd.
I will try to go dig out the photos of where I used graphite and alcohol, and did not get it all burned out.
This almost looks like what airmodel mentions, the pour was too hot, but OK85 is not prone to burn-in, at least not with cupola iron.
They do use an iron-rated pyrometer at the Metal Museum, to avoid poring too hot.
The thing about metal burning into the sand, is that it produces an additive to the castings.
These defects are negative, and into the face of the casting.
It is a bit odd that it does not occur on the perimeter.
Could have been the graphite alcohol gassing though.
.
.
CI:
This is a bearing cap I cast using identical resin and sand.
I did not have time to do much work on the pattern.
He wanted to keep the original letters, so I patched up the broken casting, but left some blue tape on it.
You can see the blue tape mirrored into the sand very accurately.
This mold had a coat of "Velacote" (tm) ceramic mold coat, which was burned off prior to pouring.
Not any odd defects like the one's Laura experienced.
I don't see any vent holes in this mold.
Normally I vent the highpoint of the mold.
Edit: Actually I do see vent holes in the cope; last photo, mold on the right side.
.
CI:
The bearing cap casting.
I did not know about spin traps when I cast this piece, but luckily it still turned out ok.
You can see the iron was quite fluid, since it rose up and out the vent holes (2nd photo).
.
CI:
This was the 2nd pour I ever made, and I made a lot of mistakes.
I was trying to use oil-based sand, and sprayed a mixture of alcohol and graphite onto the drag mold, and did not get it all burned off.
I would not suggest spraying alcohol onto oil-based sand anyway, but I had no casting experience, and so learning as I went.
The alcohol flashed and created huge bubbles.
I see some sand inclusions too.
This is a great example of how NOT to cast metal.
Almost everything that could go wrong did go wrong on the casting.
One has to start somewhere, and mistakes will be made if you are going to learn the process.
Also are photos of an ingot that was poured right after this casting was poured.
Note: Tall risers like those in the photos are not necessary; don't copy that.
No bubbling on the top of the casting because the alcohol and graphite were not used on that side.
Comparing this casting with Laura's shown above, it seems possible that her alcohol and graphite gassed.
I think the problems that showed up outside of her casting were from entrain air in the iron.
.
CI:
A camelback and straight edge I cast.
No problems with sand, etc.
Same resin-bound sand.
There was some odd surface wrinkling, I am not sure why, but that was superficial, and the edges/surfaces machined well without any inclusions or hard spots.
The patterns were made by a buddy of mine, who needed them cast in gray iron.
.